APPLICATION FILE / Surface treatment
Microscopic section measurement of anodised layers
Anodised aluminium needs local thickness; eddy-current readings scatter on curved surfaces, so a section check is needed.
The constraint
Polishing rounds the interface, and points near the edge under-read thickness.
Approach
Vertical sectioning with low-angle polishing to limit rounding, then ten equally spaced measurements per field.
- Section vertically, mount, mark the measuring face
- Grind then polish at a low angle to avoid peeling
- Ten points per field, compared with eddy current
Outcome
Section mean 18.4 µm; eddy current differed 3% on flats and 12% on curves, so its use is now restricted.
Related instruments